牌号 | 剩磁Br | 矫顽力bHc | 内禀矫顽力iHc | 最大磁能积(BH)max | 工作温 | ||||
KGs | T | KOe | KA/m | KOe | KA/m | MGOe | KJ/m3 | ℃ | |
N30 | 10.8-11.2 | 1.08-1.12 | 9.8-10.5 | 780-836 | ≥12 | ≥955 | 28-30 | 223-239 | ≤80 |
N33 | 11.4-11.7 | 1.14-1.17 | 10.5-11.0 | 836-876 | ≥12 | ≥955 | 31-33 | 247-263 | ≤80 |
N35 | 11.7-12.1 | 1.17-1.21 | 10.8-11.5 | 860-915 | ≥12 | ≥955 | 33-35 | 263-279 | ≤80 |
N36 | 11.9-12.2 | 1.19-1.22 | 10.8-11.5 | 860-915 | ≥12 | ≥955 | 34-36 | 271-287 | ≤80 |
N38 | 12.2-12.6 | 1.22-1.26 | 10.8-11.5 | 860-915 | ≥12 | ≥955 | 36-38 | 287-303 | ≤80 |
N40 | 12.6-12.9 | 1.26-1.29 | 10.5-11.0 | 836-876 | ≥12 | ≥955 | 38-40 | 303-318 | ≤80 |
N42 | 12.9-13.2 | 1.29-1.32 | 10.5-11.0 | 836-876 | ≥12 | ≥955 | 40-42 | 318-334 | ≤80 |
N43 | 13.0-13.3 | 1.30-1.33 | 10.5-11.0 | 836-876 | ≥12 | ≥955 | 41-43 | 326-342 | ≤80 |
N45 | 13.3-13.7 | 1.33-1.37 | 10.5-11.0 | 836-876 | ≥12 | ≥965 | 43-45 | 342-358 | ≤80 |
N48 | 13.8~14.2 | 1.38~1.42 | ≥10.5 | ≥835 | ≥12 | ≥955 | 46~49 | 366~390 | ≤80 |
N50 | 13.8~14.5 | 1.38~1.45 | ≥10.5 | ≥835 | ≥11 | ≥955 | 47~51 | 374~406 | ≤80 |
N52 | 14.3~14.8 | 1.43~1.48 | ≥10.8 | ≥860 | ≥11 | ≥876 | 50~53 | 398~422 | ≤80 |
内禀矫顽力(Hcj)----------------单位为奥斯特(Oe)或安/米(A/m)
使磁体的磁化强度降为零所需施加的反向磁场强度,我们称之为内禀矫顽力。内禀矫顽力是衡量磁体抗退磁能力的一个物理量,是表示材料中的磁化强度M退到零的矫顽力。在磁体使用中,磁体矫顽力越高,温度稳定性越好。
http://shyaqct.taobao.com/?search=y&scid=229347482&scname=7s%2FM%2BsXwx7%2B0xcz6INSy0M4%3D&checkedRange=true&queryType=cat&stp=7